Thermal
and Mechanical Properties of Silver (Ag, 99.999% annealed) |
|
|
|
|
|
Density=10.5 g/cc |
|
|
|
T (K) |
Thermal
Expansion |
Heat
Capacity |
Thermal Conductivity |
Emissivity |
|
Tensile Strength |
Yield Strength |
Young's Modulus |
|
(%) |
|
(J/gK) |
|
(W/cmK) |
|
|
|
(Psi) |
|
(Psi) |
|
(Psi) |
|
373 |
0.158 |
|
|
|
4.000 |
|
|
|
|
|
|
|
|
|
360 |
0.133 |
|
|
|
4.000 |
|
|
|
|
|
|
|
|
|
340 |
0.093 |
|
|
|
4.000 |
|
|
|
|
|
|
|
|
|
320 |
0.054 |
|
|
|
4.000 |
|
|
|
2.400E+04 |
|
6.50E+03 |
|
1.180E+07 |
|
300 |
0.014 |
|
|
|
4.000 |
|
0.0200 |
|
2.470E+04 |
|
6.53E+03 |
|
1.190E+07 |
|
293 |
0.000 |
|
2.36E-01 |
|
4.000 |
|
|
|
2.500E+04 |
|
6.55E+03 |
|
1.194E+07 |
|
273 |
-0.043 |
|
2.35E-01 |
|
4.000 |
|
|
|
2.600E+04 |
|
6.60E+03 |
|
1.204E+07 |
|
260 |
-0.063 |
|
2.34E-01 |
|
4.000 |
|
|
|
2.680E+04 |
|
6.70E+03 |
|
1.210E+07 |
|
240 |
-0.100 |
|
2.31E-01 |
|
4.000 |
|
|
|
2.800E+04 |
|
6.80E+03 |
|
1.220E+07 |
|
220 |
-0.138 |
|
2.28E-01 |
|
4.000 |
|
|
|
2.900E+04 |
|
7.00E+03 |
|
1.230E+07 |
|
200 |
-0.173 |
|
2.25E-01 |
|
4.000 |
|
|
|
3.030E+04 |
|
7.25E+03 |
|
1.240E+07 |
|
180 |
-0.209 |
|
2.21E-01 |
|
4.100 |
|
|
|
3.150E+04 |
|
7.50E+03 |
|
1.250E+07 |
|
160 |
-0.241 |
|
2.16E-01 |
|
4.120 |
|
|
|
3.300E+04 |
|
7.80E+03 |
|
1.260E+07 |
|
140 |
-0.275 |
|
2.09E-01 |
|
4.140 |
|
|
|
3.500E+04 |
|
8.10E+03 |
|
1.270E+07 |
|
120 |
-0.308 |
|
2.00E-01 |
|
4.160 |
|
|
|
3.700E+04 |
|
8.45E+03 |
|
1.280E+07 |
|
100 |
-0.337 |
|
1.87E-01 |
|
4.180 |
|
|
|
3.990E+04 |
|
8.70E+03 |
|
1.290E+07 |
|
80 |
-0.363 |
|
1.66E-01 |
|
4.200 |
|
0.0080 |
|
4.200E+04 |
|
9.00E+03 |
|
1.297E+07 |
|
60 |
-0.389 |
|
1.33E-01 |
|
5.000 |
|
|
|
4.500E+04 |
|
9.15E+03 |
|
1.306E+07 |
|
40 |
-0.403 |
|
7.80E-02 |
|
9.500 |
|
|
|
4.800E+04 |
|
9.30E+03 |
|
1.312E+07 |
|
20 |
-0.410 |
|
1.55E-02 |
|
52.000 |
|
|
|
5.200E+04 |
|
9.40E+03 |
|
1.318E+07 |
|
10 |
-0.412 |
|
1.80E-03 |
|
150.000 |
|
|
|
5.440E+04 |
|
9.43E+03 |
|
1.320E+07 |
|
4.2 |
-0.412 |
|
1.24E-04 |
|
130.000 |
|
0.0044 |
|
|
|
|
|
1.320E+07 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
T(K) = Temperature in Kelvin, T(C) =
Temperature in Celsius |
|
|
T (C) =
T (K) - 273 |
|
|
|
Thermal Expansion (%) = 100 x [L(T)
- L(293)] / L(293) |
|
|
|
Heat Capacity [=] 1 J/gK = 0.23864
BTU/lbm/F |
|
|
|
Thermal Conductivity [=] 1 W/cmK =
57.77 BTU/hr/ft/F |
|
|
|
Tensile and Yield
Strengths- lower bound values given |
|
|
|
Back to Property Main Page
|
|
Do You Know Someone Who Needs A Job in Engineering, Physics or Chemistry?
|
Note:
The material of this page is copyrighted.
No part of this page shall be copied, stored or reproduced without
written permission. |
|
Disclaimer:
The information of this page is provided to our best knowledge. However we are not responsible for any
potential errors in the data. |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|